Skip to content

M4 High-Speed Steel

1.3351 (M4)

Available on Request

  • EN1.3351
  • ENHS6-5-4
  • AISIM4
  • UNST11304

Cobalt-free Mo-W high-speed steel with high carbon (1.25–1.40 %) and high vanadium (3.75–4.50 %) (AISI M4, 1.3351, HS6-5-4). Its hard vanadium-rich MC carbides give higher wear resistance than M2 and M3:2; it is heat treated to a working hardness of 62–65 HRC. Supplied annealed on request for broaches, milling cutters and form tools that machine abrasive materials, and for cold-work punches.

Spectral Analysis

wt. % · ASTM A600 ranges
C
1.25–1.40
Cr
3.75–4.75
Mo
4.25–5.50
V
3.75–4.50
W
5.25–6.50

Typical ranges according to the standard, for information only. The analysis on the material certificate applies on delivery.

01Material Properties

  • Higher wear resistance than M2 and M3:2
  • Good hot hardness; secondary hardening on tempering at 540–560 °C
  • Heat treated to 62–65 HRC
  • Moderate toughness; care needed in interrupted cutting
  • Low grindability (high vanadium)
  • Powder metallurgy (PM) production gives a more uniform carbide distribution

02Applications

  • Broaches and form tools
  • Milling cutters for heavy-duty cutting
  • Cutting tools for abrasive materials
  • Cold-work punches and cutting blades
  • Planer and form knives

03Delivery Condition

  • Max. 255 HB, soft annealed.
  • Conventional or powder metallurgy (PM) production can be considered on request.

04Heat Treatment

Heat Treatment Steps

HardeningTemperatureTime →1. preheat~500 °C2. preheat~850 °C3. preheat~1050 °CAustenitise1190–1230 °C

Quench: Oil, hot bath + air, or pressurised gas in vacuum

TemperingTemperatureTime →1. temper540–560 °C2. temper540–560 °C3. temper540–560 °C
Stages and temperatures are typical values; soaking times depend on section size.

Tempering Diagram

200 °C → 63 HRC300 °C → 62 HRC400 °C → 62 HRC500 °C → 64 HRC525 °C → 64.5 HRC550 °C → 65 HRC575 °C → 64 HRC600 °C → 62 HRC650 °C → 57 HRC0100200300400500600700505560657075Tempering temperature [°C]Hardness [HRC]1.3351 (M4)Heat treatment: 1190–1230 °CQuench: Oil
Typical hardness versus tempering temperature after hardening from 1190–1230 °C (approximate, producer data).

Values are approximate and for information only; they vary with section size, heat and furnace conditions. Binding values are determined from the manufacturer’s data under laboratory conditions.

05Mechanical Properties

Typical values by delivery and heat-treatment condition; actual values depend on section size and heat-treatment parameters.

ConditionHardnessTensile strength Rm (MPa)Note
Soft annealed (delivery)Max. 255 HB≈ 860 (max.)Machinable condition
Hardened + triple tempered (540–560 °C)62–65 HRC—Typical service range

Typical values; at high hardness, hardness rather than tensile strength is used, and the annealed Rm value is an approximate conversion from hardness. The applicable specification and material certificate govern for orders.

06Applicable Standards & Specifications

  • ASTM A600 — High-speed tool steels (M4, UNS T11304)
  • JIS G4403 — High-speed tool steels (SKH54; similar composition, not identical)

A product specification and an inspection document are different things: e.g. AMS 4928 is a product specification, EN 10204 3.1 is a type of inspection document; one does not replace the other.

07Microstructure & Metallurgical Properties

Typical microstructure information

1.3351 (M4) is a cobalt-free tungsten-molybdenum high-speed steel with high carbon and high vanadium. Depending on the heat treatment condition, its microstructure typically consists of a tempered martensitic matrix with dispersed primary and secondary carbides, dominated by vanadium-rich MC.

Typical metallurgical characteristics

  • Tempered martensitic matrix
  • High fraction of vanadium-rich MC carbides
  • Secondary hardening on tempering at 540–560 °C
  • High wear resistance and hot hardness
  • Properties influenced by austenitising and tempering parameters
1.Typical microstructure
In the hardened and triple-tempered condition: tempered martensite, undissolved primary MC and M6C carbides and fine secondary carbides precipitated during tempering. In the soft-annealed delivery condition: spheroidised carbides in a ferritic matrix.
2.Heat treatment influence
The high austenitising temperature (1190–1230 °C) takes part of the carbides into solution; the as-quenched structure contains retained austenite. Repeated tempering at 540–560 °C produces secondary hardening and transforms the retained austenite. Annealed and hardened-and-tempered 1.3351 do not show the same microstructure.
3.Grain structure
Grain size is sensitive to austenitising temperature and time; undissolved carbides restrict grain growth, while exceeding the upper limit causes grain growth and loss of toughness.
4.Carbide / precipitate distribution
Vanadium-rich MC and tungsten- and molybdenum-rich M6C carbides; fine secondary carbides precipitate during tempering. Carbide size and distribution depend on the production route (conventional / powder metallurgy), section size and forging reduction; powder metallurgy gives finer, more uniformly distributed carbides.
5.Metallographic examination
Batch-specific metallographic examination is available upon request. A microstructure image alone does not prove chemical analysis, mechanical properties or certificate compliance.

Available technical documentation

  • Chemical composition certificate
  • Mechanical test report, where available
  • Heat treatment information, where available
  • Metallographic examination, upon request

Typical microstructure information. Actual microstructure may vary depending on manufacturing route, product form and heat treatment.

08Is there a better material?

Grades in the same material family as M4 with higher wear resistance and higher impact resistance (toughness); up to two suggestions under each heading. Which one fits depends on the application's priority requirement.

Higher wear resistance

Our list has no grade with higher wear resistance than M4 without a marked trade-off in its other critical properties.

Higher impact resistance (toughness)

Suggestions are based on the critical property levels in our grade data; an improvement in one property may require a trade-off in another. The final selection must be made by technical evaluation against operating conditions, heat treatment and specification.

For more information, browse our Technical Insights

09Move Metal Supply Options

Move Metal is not a producer; we source the grade to your specification through our international producer and supplier network. Dimensions, quantity, delivery condition and documentation requirements are reviewed together.

Product forms

  • Round bar
  • Flat bar
  • Plate
  • Cut-to-size

Documents and testing

  • EN 10204 3.1 inspection certificate (chemical analysis, delivery hardness)
  • EN 10204 3.2 inspection certificate (on request, third party)
  • Carbide distribution / microstructure evaluation (e.g. SEP 1615)
  • Decarburisation depth check
  • Ultrasonic testing, on request

Supply status: Available on Request

Request M4 Quotation

Not sure if M4 is the right material for your application?

Evaluate candidate materials by application, operating conditions and priority properties with the Material Selection Guide.

Find the Right Material

Have a material requirement?

Send us your specification, drawing or RFQ. Our team will review the requirement and identify a suitable supply option.

Request a Quote